← EAC Research / EAC 研究

A review of stress corrosion cracking of austenitic stainless steels in PWR primary water

Ulla Ehrnst´en、Peter L. Andresen、Zaiqing Que

Abstract / 摘要

Initial cases of stress corrosion cracking (SCC) in pressurized water reactors (PWRs) occurred mostly but not exclusively in stagnant areas like dead-legs, but recently more extensive IGSCC has occurred in normal free-ffowing PWR primary water. Operational experience and laboratory data reveal that the main parameters in IGSCC include cold work and weld residual strain, oxygen, and residual and applied stress. Residual strain, which arises from manufacturing, surface grinding, and welding, should be limited by optimizing manufacturing procedures, minimizing alignment and fft-up stresses and using high-quality weld procedures. Preventing oxygen ingress in the make-up water should be pursued. Stresses created by thermal ffuctuations (thermal mixing, low-leakage core operation, and start-ups) deserve more attention. Weld residual stress, fft-up stresses and local stresses from load follow must be maintained below the annealed yield stress. IGSCC should be considered in aging management and in-service inspection. Detection techniques capable of identifying IGSCC should be employed.

Conclusions / 结论

The key parameters that affect IGSCC in PWRs are the degree of CW/ residual deformation, oxygen content, and residual and applied stress, which are reviewed in this paper. CW or residual deformation, especially above 10%, signiffcant increases SCC initiation and growth rate in PWR primary water. Residual strain arises from manufacturing, surface grinding, and welding. The reported IGSCC incidents in PWRs in primary water share a common feature of high hardness (at the surface or in the HAZ) and high residual strains resulting from surface grinding, welding or incomplete annealing. Laboratory investigations show that the susceptibility to cracking decreases with hardness, and is relatively low for surface hardness below about 275 HV, which is lower than many national guidelines. CW or residual deformation should be limited by optimizing manufacturing procedures (including avoiding heavy surface deformation during machining and surface grinding), minimizing alignment and fft-up stresses, and using high-quality WPS. Moreover, laboratory measurements demonstrate that sustained crack growth of CW 316L stainless steel is possible in normal PWR primary water without any pollutants, and that oxygen signiffcantly in-creases the CGR. Chlorides and sulfate have a relatively small impact on IGSCC in PWRs (without oxygen), a much smaller impact than in oxidizing BWR environments. Ensuring that PWR start-up removes ox-ygen at low temperature, and operation avoid make-up water with ox-ygen is important. All sources of stress (including weld residual stress, fft-up stresses and local stresses from load following) must be considered in designs and ideally maintained below the annealed yield stress. Macro stresses and strains in the components can be affected by the pressure changes and thermal fluctuations (thermal mixing, load follow, low-leakage core operation, and start-ups/shut-downs), which can affect IGSCC initiation and CGR and deserve more attention. Although IGSCC in austenitic stainless steels in PWR primary water has been rare, the history of IGSCC shows that the incidence will rise with time, and it should be considered in aging management and in-service inspection. Detection and mitigation techniques for IGSCC in PWRs should be employed and further developed.